Results
--
Storage Oven Temperature
F
--
Reconditioning Temperature
F
--
Reconditioning Time
hr
Note: Low-hydrogen electrodes (E70XX-E120XX with -15, -16, -18 suffixes) require heated storage per AWS D1.1. E6010 cellulosic electrodes must NEVER be oven dried - this destroys the coating.
Reference
AWS D1.1 Table 5.1 Electrode Storage Requirements:
E7018 (Low-H): Storage 250-300F, Recondition 650-750F/1hr, Max exposure 4hr
E8018-C3: Storage 300F, Recondition 700-800F/1hr
E6010 (Cellulosic): Room temp ONLY - never oven dry
E6013 (Rutile): 100F storage, 250-300F reconditioning
Max reconditions: 1-3 times per AWS D1.1